Stainless steel process piping and vessel
Benchmark data

Brine evaporator metallurgy & chloride stress corrosion limits

316L, 2205 duplex, 2507 super duplex, titanium Grade 2 and 7/12, and Hastelloy C-276 compared by UNS, PREN, Cl-SCC temperature limit and typical evaporator zone, with an interactive screening filter.

  • 6alloys
  • 50–60°C316L Cl-SCC onset
  • > 190°CC-276 immunity

Alloy screening filter

Enter the hottest wetted temperature, the bulk chloride in that zone and whether surfaces see wet-dry cycling. The filter applies the limits in the reference table below.

°C
ppm Cl⁻
AlloyScreening resultReason

Screening logic only; confirm with supplier corrosion data, crevice geometry, pH, oxygen and fluoride content.

Reference table

AlloyUNSPRENCl-SCC behaviorScreening temperature limitDry-out sensitivityTypical evaporator zones
Type 316L stainlessS3160323–25Susceptible above 50–60°C at as little as 10–100 ppm Cl⁻ under evaporative dry-out≤ 50°C (122°F), low chloride onlyHighly sensitiveAmbient pretreatment piping, low-chloride utilities; not for hot brine
Alloy 2205 duplexS32205≥ 34Resistant in moderate bulk chloride to 100–110°C; risky in concentrated dry-out films≤ 100–110°C (212–230°F), moderate chlorideSensitiveMembrane skids, HPRO/OARO pressure piping, tanks
Alloy 2507 super duplexS32750≥ 42Reliable in high-chloride brine to 100–120°C; sigma-phase risk above ~120°C≤ 100–120°C (212–248°F)ModerateOARO high-pressure piping, MVR vapor bodies at moderate temperature
Titanium Grade 2R50400n/aImmune to Cl-SCC across aqueous chloride concentrations; crevice corrosion is the limit≤ 100–120°C for crevice; upgrade aboveLowMVR heat-exchanger tubes, brine concentrator tube bundles
Titanium Grade 7 / 12R52400 / R53400n/aPd or Mo-Ni additions extend crevice-corrosion resistance above 120–130°CAbove 120–130°C where Gr. 2 crevice risk appearsLowCrystallizer heaters, hot crevice-prone zones, gasketed joints
Hastelloy C-276N10276n/a (Ni-base)Immune to Cl-SCC above 190°C (374°F+)> 190°C (374°F+)Very lowSevere ZLD crystallizers, high-scaling zones, acid-cleaning loops

Why chloride stress corrosion cracking dominates

Chloride stress corrosion cracking (Cl-SCC) needs three things at once: tensile stress (residual welding stress is enough), chloride, and temperature above the alloy's threshold. Evaporators supply all three, and dry-out concentrates chloride on the metal surface far above the bulk value. That is why 316L that survives in a 40°C RO skid fails within months in a 100°C brine concentrator, and why "bulk chloride" alone understates the risk.

PREN and its limits

The pitting resistance equivalent number (PREN = %Cr + 3.3 × %Mo + 16 × %N) ranks stainless and duplex grades for pitting and crevice resistance. It does not predict Cl-SCC for nickel alloys or titanium, which are listed as n/a. Use PREN to compare 316L, 2205 and 2507; use temperature limits for the rest.

Typical zone-by-zone selection

  • Membrane skids (<45°C): 2205 duplex or 2507 for high-pressure OARO/HPRO piping; FRP for low-pressure lines.
  • MVR brine concentrator (~95–110°C): titanium Grade 2 tubes; 2507 or titanium-clad vapor body depending on chloride.
  • Crystallizer (~110–130°C+): titanium Grade 7/12 heater tubes, Hastelloy C-276 in the hottest, most scaling-prone and acid-cleaned zones.

The mass balance modeler suggests a stage-by-stage alloy from your chemistry and endpoint.

Send us the stream before you buy the skid.

Share flow, TDS and a lab ion report. We return a preliminary mass balance, a train recommendation and the questions a vendor bid has to answer.